Part of the process guide series — see all →
Ninety percent of the die-cast aluminum parts made in China are one of two alloys, and the factories will happily pick for you. Better you pick — because the choice quietly moves your cost, your surface quality and your approval paperwork.
Ask a Chinese die-casting factory what alloy they'll use and the answer is usually "ADC12" before you finish the sentence. Ask an American drawing what it says, and it often says A380. Both are aluminum-silicon-copper workhorse alloys, both cast beautifully, and for most parts they're interchangeable — but "most" is doing real work in that sentence. Here's what actually differs, what each choice costs, and when to insist on something else.
ADC12 is the Japanese JIS H5302 standard — the default alloy across Chinese die-casting floors. A380 is its US counterpart from the ASTM B85 family. They sit in the same family: roughly 8.5–10.5% silicon for fluidity, 1.5–3.5% copper for strength, iron to keep the metal from soldering to the die. The differences are in the ranges, not the concept:
Mechanically, in cast-and-aged condition, the two land within shouting distance of each other: tensile in the low-300s MPa, yield in the mid-100s to ~170. For a housing, a bracket, a cover — the difference is noise. For a spec-controlled part, the difference is paperwork.
Not habit — supply chain. ADC12 ingot is the standard commodity in China: every melt house stocks it, price indexes are published against it, and recycled feedstock is blended for it. That makes it the cheapest and fastest alloy to run, and the one every machine on the floor is tuned for. Specifying A380 doesn't strand you — serious casters keep it for export-spec work — but expect a modest premium and sometimes a longer melt-lot lead time, because it moves in smaller volume.
There's a subtlety here worth knowing: because ADC12 is heavily recycled, composition varies between melt lots more than a textbook suggests. This is fine for most parts, and manageable everywhere — if you ask for composition certificates per heat lot and treat the alloy spec as a range you audit, not a promise you assume.
On the quote, alloy choice moves three lines: material (A380 typically a few percent above ADC12), scrap/rework risk (the wrong alloy for the finish spec shows up as rejected batches, which is far more expensive than the material premium), and paperwork (a spec-controlled alloy needs certified lots — cheap per part, non-zero per order). If a supplier's A380 quote comes back wildly higher than ADC12, ask whether they're buying virgin ingot to a cert — sometimes justified, sometimes a margin story. The honest comparison is per-part at your volume, like every other quote question covered in the sourcing process guide.
The classic failure isn't picking the wrong alloy — it's not knowing which one you got. Drawing says A380, parts arrive "equivalent", and nobody wrote it down. Protect yourself with three cheap habits:
Die-cast alloys are used as-cast — no heat treatment to lean on. Design implications worth knowing before the drawing goes out: yield in the mid-100s MPa is directional and assumes sound metal, so section changes and boss designs matter more than the datasheet; threads should be cut or use cast-in inserts rather than tapped into thin walls; and any load-carrying feature needs its margin computed against the local section, not the nominal wall. If your part genuinely needs heat-treated strength (T6-level yield), that's a conversation about moving to a different process or alloy family entirely — not about "getting better ADC12". Setting expectations here prevents the classic discovery in testing that the housing flexes where the CAD said it wouldn't.
Alloy problems usually start with vague material callouts. These are the lines that survive contact with a Chinese die-casting floor:
One sentence each, and the whole class of silent-substitution failures disappears — because the deviation now needs your signature instead of a shipping notice.
If you're evaluating moving a machined part to die casting, the alloy decision rides along. Machined parts inherit wrought-alloy habits: 6061-T6 properties, anodized finishes, welded assemblies. The die-cast equivalent rarely matches all three — ADC12 is stronger as-cast but not anodize-friendly, and the 6061 habits don't transfer. The clean way to run the comparison: price the cast version in its best-fit alloy with a finish that suits casting (conversion coating + paint, or powder), and compare that stack against the machined part as-built. Comparing "A380 + anodize" against "6061 + anodize" understates the casting unfairly; comparing each route in its best configuration gives the honest answer. A real switch that paid −50% is documented in the CNC-to-die-cast case study.
Alloy selection is a two-minute conversation that prevents the two most common die-casting disappointments: blotchy anodize and silent substitutions. I match the alloy to the part's real requirements — finish, environment, spec chain — before RFQs go out, verify the melt-lot certs at first article, and keep the die-casting partners I work with honest on the composition ranges. One accountable engineer from drawing to qualified delivery.
Die casting in China: the full capability guide →
Get the drawing right first: the DFM checklist →
Send a drawing — alloy call reviewed free →
Both alloys run in the same partner shop; the die casting factory page shows the casting range (20 g to 3 kg) and where alloy substitution gets caught before the run.
Send the drawing — I'll check the alloy call against the finish, environment and spec chain before you quote.